Home Page Profile of Company Introduction to Products Equipments & Facitities Quality Controlling Contact Us
 
 

Typical SAW Properties of Conventional Piezoelectric Crystals

 

Crystal Cut Type SAW Velocity Electromechanical Coupling Factor TCV   TCD     
Vs(m/sec) K (%) TCV(10-6/ºC) TCD(10-6/ºC)
LiNbO3 127.86º Y - X 3970 5.5 -60 78
Y - Z 3485 4.3 -85 95
LiTaO3 X - 112º Y 3295 0.75 -16.5 22.3
Y - Z 3230 0.66   35
Bi12GeO20 [110] - [001] 1264 0.70 -105 128
[001] - [110] 1680 1.30 -117 140
Li2B4O7 45º X - Z 3380 1.0   0
X - Z 3542 1.0   0
Bi12SiO20 [001] - [110] 1622 0.62 -118  
SiO2 36º Y - Z 3130 0.1   0